| Alloy Type | Rolls-Royce | Snecma | GE | Honeywell | Others |
|---|---|---|---|---|---|
| 17/4PH | - | - | - | - | - |
| Jethete | MSRR6643 | - | - | - | - |
| Maraging Steel | - | - | - | - | NGMS 800 |
| N155 | - | - | - | - | Multimet |
| Alloy Type | Al | B | C | Nb | Co | Cr | Fe | Mn | Mo | Ni | Si | Ta | Ti | W | ZR | Others |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 17/4PH | - | - | 0.04 | - | - | 16.0 | Bal | 0.04 | - | 4.0 | 0.70 | - | - | - | - | Cu 3.20, Nb+Ta 0.25 |
| Jethete | - | - | - | - | 1.5 | 11.7 | Bal | - | 1.7 | 2.8 | - | - | - | - | - | V 0.3, N 0.03 |
| Maraging Steel | - | - | - | - | 10.3 | - | Bal | - | 4.7 | 16.8 | - | - | 0.3 | - | - | - |
| N155 | - | - | - | - | 19.5 | 21.0 | Bal | - | 3.0 | 20.0 | - | - | - | 2.5 | - | N 0.14 |
| Alloy Type | Rolls-Royce | Snecma | GE | Honeywell | Others |
|---|---|---|---|---|---|
| AIRESIST 319 | - | - | - | EMS 55455 | - |
| B1900 | - | - | - | - | PWA1402, MTS1083 |
| B1914 | - | - | - | - | - |
| C1023 | MSRR7046 | - | - | - | - |
| C130 | MSRR7045 | - | - | - | - |
| C242 | MSRR7217 | - | - | - | - |
| C263 | MSRR7040 | DMD442-32 | - | - | - |
| CHS70 | - | - | - | - | - |
| CHS88 | - | - | - | - | - |
| CHS104 | - | - | - | - | - |
| CNK7 | - | - | - | - | - |
| GMR235 | - | - | - | - | - |
| GDT111 | - | - | B50A719 | - | - |
| GTD111DS | - | - | B50A858 | - | - |
| GTD222 | - | - | B50A850 | - | - |
| GTD241 | - | - | B50A972 | - | - |
| GTD262 | - | - | B50A985 | - | - |
| GTD741 | - | - | B50A973 | - | - |
| Alloy X | MSRR721 | - | - | - | - |
| Haynes 230™ | MSRR7269 | - | - | - | PWA1474 |
| Haynes 282™ | - | - | - | - | - |
| IN100 | MSRR7047 | DMD432-32 | C5OTF107 E | MS55425 | PWA658 |
| IN600 | - | - | - | - | - |
| IN625 | MSRR7198 | - | B50TF107 | EMS55425 | PWA1465 |
| IN713C | MSRR7164 | DMD421.22 | B50TF16 | EMS55371 | PWA655, PWA649 |
| IN713LC | MSRR7048 | - | B50TI239 | EMS55079 | - |
| IN718 | MSRR7132 | DMD423.32 | C5TF89 | EMS55458 | PWA649, PWA1451 |
| IN718SQ | MSRR7228 | - | - | - | - |
| IN738C | MSRR7133, 7125 | - | B50A563A | - | PWA1451 |
| IN738LC | MSRR7168, 7173 | - | B50A563B | EMS55445 | - |
| IN792-5A | MSRR7169, 7239 | - | - | - | - |
| IN939 | - | - | - | - | MTS1348, HXLM00424 |
| MM002 | MSRR7101, 7080, 7150 | - | - | - | - |
| MM246 | MSRR7061, 7062 | - | - | - | - |
| MM247 | - | - | - | EMS55447 | MTS1206 |
| M247LC | - | - | - | - | - |
| MM421 | - | - | - | - | M3612 |
| N75 | MSRR7004 | - | - | - | - |
| N80 | NSRR1077 | - | - | - | - |
| N90 | MSRR1789 | - | - | - | - |
| PE10 | MSRR7184 | - | - | - | PWA1056 |
| PWA1056 | - | - | - | - | PWA1056 |
| PWA1188 | - | - | - | - | PWA1188 |
| PWA1422 | - | - | - | - | PWA1422 |
| PWA1432 | - | - | - | - | PWA1432 |
| PWA1437 | - | - | - | - | PWA1437 |
| PWA1440 (SC) | - | - | - | - | PWA1440 |
| PWA1455 | - | - | - | - | PWA1455 |
| PWA1467 | - | - | - | - | PWA1467 |
| PWA1475 | - | - | - | - | PWA1475 |
| PWA1480 (SC) | - | - | - | - | PWA1480 |
| PWA1483 | - | - | - | - | PWA1483 |
| PWA1484 (SC) | - | - | - | - | PWA1484 |
| Rene 41 | - | - | B50TF37 | - | - |
| Rene 77 | - | DMD437.32 | C50TF15 | - | - |
| Rene 80 | - | - | C50TF47 | - | PWA1449 |
| Rene 108 | - | - | - | - | B50TF262 |
| Rene 125 | - | - | C50TF60 | - | - |
| Rene 142 | - | - | C50TF94 | - | - |
| Rene 220 | - | - | C50TF91 | - | - |
| Rene N2 | - | - | C50TF121 | - | - |
| Rene N4 | - | - | C50TF75 | - | - |
| Rene N5 | - | - | C50TF122 | - | - |
| Rene N6 | - | - | C50TF114 | - | - |
| Rene N500 | - | - | C50TF129 | - | - |
| Rene N515 | - | - | C50TF130 | - | - |
| SX-4 | - | - | - | - | - |
| SRR99 | MSRR7210 | - | - | - | MTS1162 |
| RR2000 | MSRR7225 | - | - | - | - |
| U500 | - | - | B50A467 | - | - |
| U700 | - | - | B50A524 | - | PWA656 |
| WASPALOY | - | - | - | - | PWA1471 |
| Alloy Type | Al | B | C | Nb | Co | Cr | Fe | Mn | Mo | Ni | Si | Ta | Ti | W | ZR | Others |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| AIRESIST 319 | 5.30 | 0.010 | 0.18 | 2.0 | - | 13.0 | - | - | 4.2 | Bal | - | - | 0.8 | - | 0.07 | - |
| B1900 | 6.00 | 0.015 | 0.10 | - | 10.0 | 8.0 | - | - | 6.0 | Bal | - | 4.3 | 1.0 | - | 0.07 | - |
| B1914 | 5.50 | 0.100 | - | - | 10.0 | 10.0 | - | - | 3.0 | Bal | - | - | 5.3 | - | - | - |
| C1023 | 4.10 | 0.006 | 0.15 | - | 9.7 | 15.5 | - | - | 8.0 | Bal | - | - | 3.6 | - | - | - |
| C130 | 0.85 | - | 0.06 | - | - | 21.5 | - | - | 9.8 | Bal | - | - | 2.6 | - | - | - |
| C242 | 0.15 | - | 0.31 | - | 10.0 | 21.0 | - | 0.35 | 10.5 | Bal | 0.35 | - | 0.2 | - | - | - |
| C263 | 0.50 | - | 0.06 | - | 20.0 | 20.0 | - | - | 5.8 | Bal | - | - | 2.2 | - | - | - |
| CHS70 | 3.00 | - | 0.09 | 0.2 | 10.5 | 15.5 | - | - | 1.9 | Bal | - | - | 4.5 | 5.2 | 0.02 | - |
| CHS88 | 3.40 | 0.080 | 0.07 | 0.1 | 10.5 | 15.9 | - | - | 1.9 | Bal | - | - | 4.6 | 5.3 | - | Hf 0.30 |
| CHS104 | 2.50 | 0.013 | 0.11 | 0.3 | 11.0 | 21.0 | - | - | 0.6 | Bal | - | - | 3.5 | 3.5 | - | - |
| CNK7 | 3.40 | 0.012 | 0.12 | - | 4.5 | 13.2 | - | - | 0.7 | Bal | - | - | 4.7 | 7.0 | - | - |
| GMR235 | 3.60 | 0.050 | 0.15 | - | - | 15.5 | 10.00 | 0.30 | 5.0 | Bal | 0.40 | - | 2.0 | - | - | - |
| GDT111 | 3.00 | 0.010 | 0.10 | - | 9.5 | 14.0 | - | - | 1.5 | Bal | - | 2.8 | 4.9 | 3.8 | 0.01 | - |
| GTD111DS | 3.00 | 0.010 | 0.10 | - | 9.5 | 14.0 | - | - | 1.5 | Bal | - | 2.8 | 4.9 | 3.8 | <0.01 | - |
| GTD222 | 1.20 | 0.010 | 0.10 | 0.8 | 19.0 | 22.5 | - | - | - | Bal | - | 1.0 | 2.3 | 2.0 | 0.02 | - |
| GTD241 | 1.20 | 0.004 | 0.10 | - | 19.0 | 22.5 | - | - | - | Bal | - | - | 2.3 | 2.0 | 0.01 | Nb+0.508Ta 1.3 |
| GTD262 | 1.70 | 0.006 | 0.01 | - | 19.0 | 22.5 | - | - | - | Bal | - | - | 2.3 | 2.0 | 0.01 | Nb+0.508Ta 1.35 |
| GTD741 | 3.50 | 0.012 | 0.10 | - | 8.5 | 16.0 | - | - | 1.8 | Bal | - | - | 3.5 | 2.6 | 0.02 | Nb+0.508Ta 1.8 |
| Alloy X | - | 0.800 | 0.08 | - | 22.0 | 18.5 | - | 0.50 | 8.5 | Bal | 0.08 | - | - | 0.6 | - | - |
| Haynes 230™ | 0.35 | 0.005 | 0.07 | - | - | 22.0 | - | 0.60 | 2.0 | Bal | 0.45 | - | - | 14.0 | - | - |
| Haynes 282™ | 1.55 | 0.006 | 0.06 | - | 10.0 | 20.5 | 1.50 | - | 8.5 | Bal | - | - | 2.1 | - | - | - |
| IN100 | 5.50 | 0.015 | 0.17 | - | 15.0 | 9.7 | - | - | 3.0 | Bal | - | - | 4.7 | - | 0.04 | V 0.9 |
| IN600 | - | - | 0.10 | - | - | 15.5 | 8.00 | 0.80 | - | Bal | 0.30 | - | - | - | - | - |
| IN625 | 0.20 | - | 0.05 | 3.6 | - | 21.5 | 3.00 | 0.20 | 9.0 | Bal | 0.20 | - | 0.2 | - | - | - |
| IN713C | 6.00 | 0.010 | 0.15 | 2.2 | - | 13.5 | <2.00 | - | 4.2 | Bal | - | - | 0.8 | - | 0.07 | - |
| IN713LC | 6.00 | 0.010 | 0.06 | 2.0 | - | 12.0 | - | - | 4.2 | Bal | - | - | 0.8 | - | - | - |
| IN718 | 0.60 | - | 0.06 | - | - | 19.0 | Bal | - | 3.0 | 52.5 | - | - | 0.9 | - | - | Cb+Ta 5.0 |
| IN718SQ | 0.60 | - | 0.06 | - | - | 19.0 | Bal | - | 3.0 | 52.5 | - | - | 0.9 | - | - | Cb+Ta 5.0 |
| IN738C | 3.40 | 0.010 | 0.17 | 0.8 | 8.4 | 16.0 | - | - | 1.7 | Bal | - | 1.8 | 3.4 | 2.6 | 0.06 | - |
| IN738LC | 3.40 | 0.010 | 0.10 | 0.8 | 8.4 | 16.0 | - | - | 1.7 | Bal | - | 1.8 | 3.4 | 2.6 | 0.03 | - |
| IN792-5A | 3.40 | 0.015 | 0.08 | - | 9.0 | 12.6 | - | - | 2.0 | Bal | - | 4.0 | 4.0 | 4.0 | 0.03 | - |
| IN939 | 1.90 | 0.010 | 0.15 | 1.0 | 19.0 | 22.5 | - | - | - | Bal | - | 1.4 | 3.7 | 2.0 | 0.09 | - |
| MM002 | 5.50 | 0.015 | 0.15 | - | 10.0 | 9.0 | - | - | - | Bal | - | 2.5 | 1.5 | 10.0 | 0.04 | Hf 1.4 |
| MM246 | 5.50 | 0.015 | 0.15 | - | 10.0 | 9.0 | - | - | 2.5 | Bal | - | 1.5 | 1.5 | 10.0 | 0.05 | - |
| MM247 | 5.50 | 0.015 | 0.15 | - | 10.0 | 8.4 | - | - | 0.7 | Bal | - | 3.1 | 1.0 | 10.0 | 0.04 | Hf 1.4 |
| M247LC | 5.60 | 0.015 | 0.07 | - | 9.3 | 8.1 | - | - | 0.5 | Bal | - | 3.2 | 0.7 | 9.5 | 00.1 | Hf 1.4 |
| MM421 | 4.20 | 0.015 | 0.15 | 1.8 | 10.0 | 15.8 | - | - | 2.0 | Bal | - | - | - | - | - | - |
| N75 | 0.20 | - | 0.12 | - | - | 19.5 | - | 0.60 | - | Bal | 0.60 | - | 0.4 | - | - | - |
| N80 | 1.20 | - | 0.07 | - | - | 20.0 | - | 0.60 | - | Bal | 0.60 | - | 2.6 | - | - | - |
| N90 | 1.20 | - | 0.09 | - | 16.0 | 20.0 | - | 0.60 | - | Bal | 0.60 | - | 2.6 | - | - | - |
| PE10 | - | - | 0.04 | 6.7 | - | 20.0 | 3.00 | 0.30 | 6.0 | Bal | 0.25 | - | - | 2.5 | - | - |
| PWA 1056 | - | - | - | - | - | - | - | - | - | Bal | - | - | - | - | - | - |
| PWA 1188 | 3.40 | 0.025 | 0.05 | 0.9 | 20.3 | 13.0 | - | - | 3.8 | Bal | - | 2.4 | 3.7 | 2.1 | 0.05 | - |
| PWA 1422 | 5.00 | 0.015 | 0.14 | 1.0 | 10.0 | 9.0 | - | - | - | Bal | - | - | 2.0 | 12.0 | - | 1.6Hf |
| PWA 1432 | 3.50 | 0.012 | 0.11 | - | 9.0 | 12.2 | - | - | 1.9 | Bal | - | 5.0 | 4.1 | 3.8 | 0.004 | - |
| PWA 1437 | 3.60 | 0.012 | 0.11 | - | 9.0 | 12.1 | - | - | 1.9 | Bal | - | 5.0 | 4.1 | 3.8 | <0.02 | - |
| PWA 1440 (SC) | 5.00 | 0.003/mx | 0.04 | - | 5.0 | 10.0 | - | - | - | Bal | - | 12.0 | 1.5 | 4.0 | 0.03/mx | Hf 0.35 |
| PWA 1455 | 6.00 | 0.015 | 0.10 | - | 10.0 | 8.0 | - | - | 6.0 | Bal | - | 4.3 | 1.0 | - | 0.04 | Hf 1.1 |
| PWA 1467 | 3.40 | 0.015 | 0.12 | - | 9.0 | 12.4 | - | - | 2.1 | Bal | - | 4.2 | 4.0 | 4.0 | 0.06 | Hf 0.5 |
| PWA 1475 | 6.60 | 0.007 | 0.10 | - | - | 10.0 | - | - | 2.0 | Bal | - | 4.1 | - | 3.2 | 0.3 | Hf 1.2 |
| PWA 1480 (SC) | 5.00 | 0.003/mx | 0.05/mx | - | 5.0 | 10.0 | - | - | - | Bal | - | 12.0 | 1.5 | 4.0 | 0.015/mx | - |
| PWA 1483 | 3.60 | 0.003/mx | 0.07 | - | 9.0 | 12.2 | - | - | 1.9 | Bal | - | 5.0 | 4.1 | 3.8 | 0.0075/mx | - |
| PWA 1484 (SC) | 5.60 | 0.003/mx | 0.05/mx | - | 10.0 | 5.0 | - | - | 1.9 | Bal | - | 8.7 | - | 6.0 | 0.015/mx | Re 3.0 Hf 0.1 |
| R41 | 1.65 | 0.006 | 0.09 | - | 11.0 | 19.0 | - | - | 9.5 | Bal | - | - | 3.1 | - | - | - |
| R77 | 4.30 | 0.015 | 0.07 | - | 15.0 | 14.7 | - | - | 4.2 | Bal | - | - | 3.4 | - | 0.04 | - |
| R80 | 3.00 | 0.015 | 0.17 | - | 9.4 | 14.0 | - | - | 4.0 | Bal | - | - | 5.0 | 4.0 | 0.02 | - |
| R108 | 5.50 | 0.015 | 0.08 | - | 9.5 | 8.4 | - | - | 0.5 | Bal | - | 3.0 | 0.8 | 9.5 | 0.01 | Hf 1.5 |
| R125 | 4.80 | 0.015 | 0.11 | - | 10.0 | 8.9 | 8.9 | 8.9 | 2.0 | Bal | - | 3.8 | 2.4 | 7.0 | 0.04 | Hf 1.6 |
| R142 | 6.10 | 0.015 | 0.12 | - | 11.8 | 6.8 | - | - | 1.5 | Bal | - | 6.4 | 0.02/mx | 4.9 | 0.03/mx | Hf 1.5 Re 3.0 |
| R220 | 0.50 | 0.004 | 0.03 | 5.3 | 12.0 | 19.0 | - | - | 3.2 | Bal | - | 3.3 | 1.0 | - | - | - |
| N2 | 6.60 | 0.004 | 0.04 | - | 7.51 | 3.0 | - | - | - | Bal | 0.05 | 5.0 | 0.04/mx | 3.8 | 0.015/mx | Hf 0.1 Re 1.6 |
| N4 | 4.20 | 0.004 | 0.06 | 0.5 | 7.5 | 9.8 | - | - | 1.5 | Bal | - | 4.8 | 3.5 | 6.0 | - | Hf 0.15 |
| N5 | 6.20 | 0.004 | 0.05 | - | 7.5 | 7.0 | - | - | 1.5 | Bal | - | 6.5 | 0.04/mx | 5.0 | - | Hf 0.15 Re 3.0 |
| N6 | 5.80 | 0.004 | 0.05 | - | 12.5 | 4.2 | - | - | 1.4 | Bal | - | 7.2 | 0.04/mx | 6.0 | - | Hf 0.15 Re 5.4 |
| N500 | 6.60 | 0.004 | 0.04 | - | 7.5 | 6.0 | - | - | 1.5 | Bal | - | 6.6 | 0.04/mx | 6.3 | - | Hf 0.15 |
| N515 | 6.30 | 0.004 | 0.05 | - | 7.5 | 6.0 | - | - | 2.0 | Bal | - | 6.5 | 0.04/mx | 6.3 | - | Hf 0.6 Re 1.5 |
| SX-4 | 5.60 | - | 0.006/mx | - | 9.6 | 6.4 | - | - | 0.6 | Bal | - | 6.5 | 1.0 | 6.4 | - | Hf 0.09 Re 2.95 |
| SR99 | 5.50 | - | 0.02 | - | 5.1 | 8.5 | - | - | - | Bal | - | 2.8 | 2.2 | 9.4 | - | - |
| RR2000 | 5.50 | - | 0.015 | - | 15.0 | 10.0 | - | - | 3.0 | Bal | - | - | 4.0 | - | - | V 1.0 |
| U500 | 3.00 | 0.008 | 0.08 | - | 17.5 | 19.0 | - | - | 4.0 | Bal | - | - | 2.9 | - | - | - |
| U700 | 4.30 | 0.020 | 0.80 | - | 15.0 | 15.0 | - | - | 4.5 | Bal | - | - | 3.3 | - | - | - |
| WASPALOY | 1.10 | 0.005 | 0.07 | - | 13.5 | 19.5 | - | - | 4.3 | Bal | - | 3.0 | - | - | 0.07 | - |
| Alloy Type | Rolls-Royce | Snecma | GE | Honeywell | Others |
|---|---|---|---|---|---|
| CoCrMo | - | - | - | - | HS21, ASTM F75 |
| ECY768 | - | - | - | - | HS21, ASTM F75 |
| FSX414 | - | - | B50A910 | - | - |
| X40 | MSRR7049, 7122 | DMD403.32 | C50TF21 | - | HS31, PWA648 |
| X45 | - | DMD405.32 | B50A3744B | - | - |
| MM302 | - | - | - | - | PWA657 |
| MM509 | - | DMD.401-32 | B50TF89 | EMS55451 | PWA647 |
| Alloy Type | Al | B | C | Nb | Co | Cr | Fe | Mn | Mo | Ni | Si | Ta | Ti | W | ZR | Others |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| CoCrMo | - | - | 0.23 | - | Bal | 28.0 | - | 0.50 | 6.0 | - | 0.80 | - | - | - | - | - |
| ECY768 | 0.20 | - | 0.60 | - | Bal | 23.5 | - | - | - | 10.0 | - | 3.5 | 0.2 | 7.0 | - | - |
| FSX414 | - | 0.100 | 0.25 | - | Bal | 29.5 | - | 0.70 | - | 11.0 | 0.90 | - | - | 7.0 | - | - |
| X40 | - | - | 0.50 | - | Bal | 25.5 | - | 0.80 | - | 10.5 | 0.80 | - | - | 7.5 | - | - |
| X45 | - | 0.100 | 0.25 | - | Bal | 25.5 | - | 0.50 | - | 10.5 | 0.80 | - | - | 7.5 | - | - |
| MM302 | - | 0.005 | 0.85 | - | Bal | 21.5 | - | - | - | - | - | 9.0 | - | 10.0 | 0.02 | - |
| MM509 | - | - | 0.60 | - | Bal | 23.5 | - | - | - | 10.0 | - | 3.5 | 0.2 | 7.0 | 0.45 | - |